Skip to content
Back to the journal

Fabrication Process

Metal Surface Finishing: The Complete In-Depth Process Guide — Spray, Polish, Brush and Electroplate in 4 Processes, 32 Sub-Processes, 12 Defect Types and 6 Inspection Groups

Spray color 60–120µm; polish gloss 8K; brush grain 80–400#; plate wear 1–30µm. GU 10/30–60/60–85/95/8K. Line: clear 180℃, grit 2800rpm, grain/passivate, degrease/plate/seal. Scene: hall polish/plate, room brush/matte, ext plate/spray. Check: film, gloss, X-cut, 2H, salt, ΔE. Defects: particle/sag/peel/drift/thin/scratch/mark/burn/blister/adhesion/yellow/prints; fix: filtration, media, bath, seal.

By GUOYAO METALPublished Updated 20 min read
Metal surface finishing in the field: mirror-polished, brushed and PVD gold titanium finished panels combined on one elevation.

Luxury boutiques, high-end residences and luxury hotels ask very different things of metal surface finishing, yet they share one underlying logic: pre-treatment decides adhesion, process parameters decide texture, and process control decides batch consistency. This guide breaks spray coating, polishing, brushing and electroplating down to the sub-process level, with a scene selection matrix, parameter gradients, equipment configuration, inspection methods and defect prevention.

Headline figures for the whole system:

  • Core processes: 4 — spray · polish · brush · electroplate
  • Sub-processes detailed: 32
  • Minimum mirror roughness: Ra 0.01 μm
  • PVD film thickness range: 0.3–0.5 μm
  • Retail colour-difference control: ΔE ≤ 0.8
  • Salt-spray benchmark: ≥ 500 h
  • Defect types covered: 12
  • Inspection groups: 6

1. The Four Surface Treatment Processes at a Glance

Spray for colour, polishing for gloss, brushing for texture, plating for performance. The four processes can be used alone or stacked in combination — selection depends on the base material, the scene and the budget, but the pre-treatment logic and quality-control principles are the same.

1.1 Spray Coating

Spray booth in the field: an operator spraying an aluminium panel with an electrostatic gun
Spray booth in the field: an operator spraying an aluminium panel with an electrostatic gun

Atomised paint is sprayed onto the metal surface to form a continuous coating. Strong colour capability across the full matte-to-gloss range — the workhorse process for aluminium panels and shaped parts.

  • Film — 30–120 μm
  • Colour difference — ΔE ≤ 1.0
  • Best for — aluminium / shaped parts

1.2 Polishing

8K mirror-polished stainless steel: distortion-free reflection
8K mirror-polished stainless steel: distortion-free reflection

Microscopic peaks are removed mechanically or chemically to lower roughness. From matte satin to an 8K mirror, the polish grade directly decides the metal's sense of quality.

  • Roughness — Ra 0.01–0.8 μm
  • Gloss — 12–96 GU
  • Best for — stainless / copper

1.3 Brushing

Long-grain brushed stainless steel panel: directional hairline texture
Long-grain brushed stainless steel panel: directional hairline texture

Abrasives scratch the surface in a controlled direction to form a regular pattern. Brushing hides fine scratches, cuts reflection and adds tactile depth — the most widely used metal texture process for residences and hotels.

  • Roughness — Ra 0.2–1.2 μm
  • Texture — long / short / snow grain
  • Best for — all scenes

1.4 Electroplating / PVD

PVD gold titanium coated panel: hard metallic colour finish
PVD gold titanium coated panel: hard metallic colour finish

A metal layer is deposited by electrolysis or vacuum coating. PVD titanium coating gives gold, black titanium, rose gold and other colours with high hardness and wear and corrosion resistance — the first choice for luxury boutiques.

  • Film — 0.3–0.5 μm
  • Hardness — HV 1500–2500
  • Best for — retail / hotel

Key point: the four processes are not interchangeable. Spray changes colour, polish changes gloss, brush changes texture and plate changes performance — pick the property you actually need before you pick the process.

2. The Gloss Scale and Process Usage Split

Gloss is the first thing the eye reads, and it is the parameter most often left unquantified on drawings. Measured in 60° gloss units (GU), higher values reflect more. Luxury boutiques take the high range, high-end residences the mid-to-low range, and hotels grade it zone by zone.

2.1 Gloss Level at 60°

Gloss scale sample panels: from matte shot-blasted to 8K mirror
Gloss scale sample panels: from matte shot-blasted to 8K mirror
  • 8K mirror polish — 96 GU · Ra ≤ 0.01 μm
  • Satin polish — 68 GU · Ra 0.10 μm
  • Fine short-grain brushed — 52 GU · Ra 0.30 μm
  • Long-grain brushed (snow-fine) — 38 GU · Ra 0.50 μm
  • Matte shot-blasted — 12 GU · Ra 1.20 μm
  • Chemical etched texture — 6 GU · Ra 2.00 μm
  • Fluorocarbon spray (matte) — 4 GU · Ra 2.50 μm

Gloss scale, physical samples — left to right: matte shot-blasted 12 GU · brushed 30–55 GU · satin 68 GU · 8K mirror 96 GU. Gloss and roughness Ra correspond one to one; boutiques take the high end, residences the mid-to-low end, hotels grade by zone.

2.2 Process Usage Split

Four finished panels side by side: spray coated, mirror polished, brushed and PVD plated
Four finished panels side by side: spray coated, mirror polished, brushed and PVD plated

Actual usage frequency of the four processes, sampled across mid-to-high-end architectural metal finishing projects.

  • Brushing — 35%
  • Electroplating — 25%
  • Polishing — 22%
  • Spraying — 18%

Key point: brushing is the most used process overall, but usage split is not the same as budget split — PVD plating is the smallest share by area and the largest by cost.

3. Spray Coating: The Complete Process

The heart of spraying is not the spraying but the pre-treatment and curing. Coating adhesion, colour difference and weatherability depend seven-tenths on thorough pre-treatment and a precise cure curve. Broken down below from substrate pre-treatment to finished-part inspection.

3.1 Process Flow

Atomised paint is attached evenly to the metal surface, then levelled and cured into a continuous coating. Suited to aluminium panels, shaped parts and large facades, with the full colour range from matte to gloss and from plain to metallic. Common types: fluorocarbon (PVDF), powder and ceramic coating.

  • Step 01 · Substrate pre-treatment — degrease → derust → chromate
  • Step 02 · Primer spray — film 5–10 μm
  • Step 03 · Levelling & flash-off — room temperature, 10–15 min
  • Step 04 · Topcoat spray — film 25–40 μm
  • Step 05 · High-temp cure — 180–250 ℃ / 15–25 min
  • Step 06 · Cooling & inspection — ΔE / film / adhesion

3.2 Sub-Process Breakdown

Pre-treatment

  • 01-1 Alkaline degreasing — alkaline degreaser pH 9–11 · 50–60 ℃ · soak / spray 3–5 min · rinse to conductivity ≤ 50 μS/cm
  • 01-2 Acid pickling — nitric / sulfuric mixed acid · room temperature 2–5 min · removes scale and rust · two rinse stages
  • 01-3 Chromating / chromate-free passivation — chromate bath Cr³⁺ 0.5–2 g/L · 25–35 ℃ · 1–3 min · forms a nanoscale conversion film
  • 01-4 DI-water rinse & drying — DI-water rinse conductivity ≤ 10 μS/cm · drying 80–120 ℃ / 10–15 min · no water marks · into the dust-free booth

Primer

  • 02-1 Primer spray — epoxy primer film 5–10 μm · gun distance 150–250 mm · atomising pressure 0.3–0.5 MPa · even coverage, no misses

Topcoat

  • 04-1 Topcoat spray — fluorocarbon / powder film 25–40 μm · spray environment 20–28 ℃ / 45–65% RH · thin multi-pass spraying 2–3 passes · colour difference ΔE ≤ 1.0

3.3 Key Parameters

  • Pre-treatment — chromating / chromate-free passivation
  • Degrease temperature — 50–60 ℃
  • DI-water conductivity — ≤ 10 μS/cm
  • Spray environment — 20–28 ℃ · 45–65% RH
  • Gun distance — 150–250 mm
  • Atomising pressure — 0.3–0.5 MPa
  • Total film — 30–120 μm
  • Cure temperature — 180–250 ℃
  • Cure time — 15–25 min
  • Adhesion — cross-cut class 0 / ≥ 95% squares
  • Weatherability — QUV ≥ 2000 h
  • Pencil hardness — ≥ 2H

3.4 Control Points

  • Pre-treatment is everything — incomplete degreasing causes blistering and peeling. The line must run degrease → rinse → chromate → DI rinse with conductivity ≤ 10 μS/cm.
  • Layered film control — primer 5–10 μm and topcoat 25–40 μm; too thick sags, too thin lacks hiding power.
  • Same-batch colour control — one colour code must be sprayed in one batch, with every panel colorimeter-checked to ΔE ≤ 1.0.
  • Cure-curve records — oven temperature curves must be archived; too fast a ramp causes pinholes and orange peel.
  • Booth cleanliness — the booth must be positive-pressure dust-free with particles ≤ 1000/m³, or the coating shows specks.
  • Jig management — jigs need regular cleaning; residual coating affects conductivity and earthing, giving uneven film build.

3.5 Equipment

  • Pre-treatment line — degreasing / pickling tanks · chromate / DI-rinse tanks · drying oven
  • Spray equipment — electrostatic / air spray guns · reciprocators / robots · positive-pressure dust-free booth
  • Curing equipment — tunnel curing oven · oven temperature tracker · cooling zone
Spray coating cross-section (real cut edge): metal substrate, chromate conversion layer, primer, topcoat and clear coat strata
Spray coating cross-section (real cut edge): metal substrate, chromate conversion layer, primer, topcoat and clear coat strata

Spray coating cross-section (real cut edge) — metal substrate (aluminium / stainless) → chromate layer / nanoscale conversion film → primer 5–10 μm → topcoat 25–40 μm → clear coat (optional) 8–15 μm. Total film 30–120 μm · multi-pass spraying · high-temp cured · adhesion cross-cut class 0.

Spray pre-treatment line: degreasing, pickling, chromating and DI-rinse tanks
Spray pre-treatment line: degreasing, pickling, chromating and DI-rinse tanks
Alkaline degreasing tank: 50–60 ℃ soak and spray
Alkaline degreasing tank: 50–60 ℃ soak and spray
Positive-pressure dust-free spray booth: electrostatic guns and reciprocator at work
Positive-pressure dust-free spray booth: electrostatic guns and reciprocator at work
Tunnel curing oven: high-temperature film curing
Tunnel curing oven: high-temperature film curing
Coating inspection: thickness measurement and cross-hatch adhesion testing
Coating inspection: thickness measurement and cross-hatch adhesion testing

4. Polishing: The Complete Process

Polishing is a subtractive process — microscopic peaks are removed by step-by-step grinding. From coarse grinding to mirror, every grade must fully remove the previous grade's marks or a haze remains. Polish grades from matte to 8K mirror directly decide the metal's sense of quality.

4.1 Process Flow

Abrasives or chemical action lower the surface roughness to give a mirror or satin finish. Mechanical polishing steps through belts, sisal wheels and cloth wheels; electrolytic polishing dissolves electrochemically for a uniform mirror.

  • Step 01 · Coarse grind — #120–#240 belt
  • Step 02 · Medium grind — #400–#800 belt
  • Step 03 · Fine grind — #1000–#2000
  • Step 04 · Sisal buffing — compound W20–W10
  • Step 05 · Cloth-wheel finishing — compound W5–W1
  • Step 06 · Cleaning & inspection — Ra / gloss

4.2 Sub-Process Breakdown

  • 01-1 Coarse grinding — belt #120–#240 · belt speed 15–25 m/s · removes weld marks and deep scratches · direction perpendicular to the next grade
  • 02-1 Medium grinding — belt #400–#800 · pressure 0.2–0.5 MPa · removes coarse-grind marks · even surface, no patches
  • 03-1 Fine grinding — belt / paper #1000–#2000 · wet or oil grinding · uniform matte surface · prepares for buffing
  • 04-1 Sisal buffing — sisal wheel Ø 200–300 mm · speed 2000–2500 rpm · compound W20–W10 · removes fine-grind marks
  • 05-1 Cloth-wheel finishing — cloth wheel Ø 250–350 mm · speed 2500–3000 rpm · compound W5–W1 · achieves the mirror
  • 06-1 Cleaning & inspection — ultrasonic cleaning with neutral detergent · profilometer Ra check · gloss meter GU check · visual check for haze / rings

4.3 Key Parameters

  • Coarse grit — #120 – #240
  • Medium grit — #400 – #800
  • Fine grit — #1000 – #2000
  • Rough buffing speed — 2000–2500 rpm
  • Finishing buffing speed — 2500–3000 rpm
  • Compound grade — W20 – W1
  • Buffing pressure — 0.2–0.5 MPa
  • Final roughness — Ra 0.01–0.8 μm
  • Gloss — 12–96 GU
  • Flatness — ≤ 0.5 mm/m
  • Surface temperature — ≤ 80 ℃
  • Electrolytic current density — 20–50 A/dm²

4.4 Control Points

  • Step through every grit — each new belt must fully remove the previous grade's marks, or the mirror shows haze or rings.
  • Alternate direction — grind each grade perpendicular to the last so you can see at a glance whether it is ground through.
  • Temperature control — excessive pressure overheats the surface locally, yellowing stainless steel and oxidising copper.
  • Electropolishing — ideal for complex shaped parts and gives a uniform mirror, but current density and electrolyte temperature must be controlled.
  • Buffing wheel care — cloth wheels need regular dressing; an uneven wheel face causes waviness.
  • Clean immediately — clean straight after polishing; residual compound corrodes the surface.

4.5 Equipment

  • Grinding equipment — wide-belt sander · surface grinder · belt grinder
  • Polishing equipment — buffing lathes / automatic lines · sisal / cloth / wool wheels · automatic compound spraying
  • Electropolishing — electrolytic tank / rectifier · temperature control system · cathode plates / jigs
Polish grades from matte to mirror: matte, satin, half-mirror and 8K mirror
Polish grades from matte to mirror: matte, satin, half-mirror and 8K mirror

Polish grades · from matte to mirror — matte 12 GU → satin 48 GU → half-mirror 72 GU → 8K mirror 96 GU · super-mirror Ra ≤ 0.01 μm. Each step up must fully remove the previous grade's marks, or haze and rings appear.

Wide-belt sander coarse grinding: removing weld marks and deep scratches
Wide-belt sander coarse grinding: removing weld marks and deep scratches
Fine wet grinding: refining to a uniform matte surface
Fine wet grinding: refining to a uniform matte surface
Sisal wheel buffing: removing fine-grind marks
Sisal wheel buffing: removing fine-grind marks
Cloth wheel finishing: achieving the mirror effect
Cloth wheel finishing: achieving the mirror effect
8K mirror reflection test: distortion-free face-on
8K mirror reflection test: distortion-free face-on

5. Brushing: The Complete Process

Brushing forms texture by directional abrasive scratching. Grain direction, coarseness and depth decide the final look — long grain is continuous, short grain is fine, snow-fine gives a random pattern. Brushing hides fine scratches, cuts reflection and adds tactile depth.

5.1 Process Flow

Belts, non-woven pads or wire brushes scratch the metal surface directionally to form regular or random micro-texture — the most widely used metal texture process for premium residences and hotels. Grain grades include coarse, fine, long, short and snow-fine.

  • Step 01 · Substrate cleaning — degrease / dust off
  • Step 02 · Coarse grain setting — #120–#240 belt
  • Step 03 · Fine grain refining — #320–#600 belt
  • Step 04 · Grain unifying — non-woven pad / nylon wheel
  • Step 05 · Surface cleaning — remove swarf
  • Step 06 · Film protection — PE film / AF coating

5.2 Sub-Process Breakdown

  • 01-1 Substrate cleaning — wipe with neutral detergent · removes oil and fingerprints · compressed-air dusting · surface dry, no water marks
  • 02-1 Coarse grain setting — belt #120–#240 · belt speed 12–20 m/s · feed rate 3–8 m/min · sets grain direction and depth
  • 03-1 Fine grain refining — belt #320–#600 · lowers surface roughness · finer, more even grain · direction matches the coarse pass
  • 04-1 Grain unifying — non-woven pad / nylon wheel · removes belt seams · grain depth 0.5–3 μm · gloss 30–55 GU
  • 05-1 Surface cleaning — removes swarf and dust · wipe with neutral detergent · blown dry with compressed air · check grain evenness
  • 06-1 Film protection — PE protective film 50–80 μm · anti-fingerprint coating 1–3 μm · corner guards on all four edges · avoid stacking damage

5.3 Key Parameters

  • Coarse grit — #120 – #240
  • Fine grit — #320 – #600
  • Belt speed — 12–20 m/s
  • Feed speed — 3–8 m/min
  • Grain depth — 0.5–3 μm
  • Roughness — Ra 0.2–1.2 μm
  • Gloss — 30–55 GU
  • Grain direction — long / short / random
  • Anti-fingerprint coating — 1–3 μm
  • Coating hardness — ≥ 3H

5.4 Control Points

  • One grain direction — every panel on the same elevation must be brushed in the same direction, or reflections clash badly at different angles.
  • Seam transition — grain on adjacent panels must flow across the joint; the texture must not break at the seam.
  • Belt wear management — belts must be replaced at end of life, or the grain gets shallower and colour difference appears.
  • Anti-fingerprint coating — an AF coating after brushing stops fingerprints — standard for premium residences and hotels.
  • Even pressure — brushing pressure must stay constant; pressure fluctuation gives uneven grain depth.
  • Clean thoroughly — all swarf must be removed after brushing; residual dust harms later coating adhesion.

5.5 Equipment

  • Brushing equipment — wide-belt brushing machine · flat-panel brushing machine · automatic brushing line
  • Abrasives & consumables — belts #120–#600 · non-woven pad / nylon wheel · wire brushes / grinding wheels
  • Coating equipment — AF coating spray line · baking oven · film applicator
Brushed texture comparison: long grain, short grain, snow-fine and coarse grain
Brushed texture comparison: long grain, short grain, snow-fine and coarse grain

Brushed texture comparison · four typical grains — long grain (continuous · strong directionality) · short grain (fine · soft) · snow-fine (random · hides scratches well) · coarse grain (deep · industrial look). Grain depth 0.5–3 μm · one direction per elevation.

Substrate cleaning: neutral detergent and compressed-air dusting
Substrate cleaning: neutral detergent and compressed-air dusting
Coarse grain setting: fixing the grain direction and depth
Coarse grain setting: fixing the grain direction and depth
Fine grain refining: a finer, more even texture
Fine grain refining: a finer, more even texture
Grain unifying: a non-woven pad removing belt seams
Grain unifying: a non-woven pad removing belt seams
Anti-fingerprint coating line: the standard protection after brushing
Anti-fingerprint coating line: the standard protection after brushing

6. Electroplating & PVD: The Complete Process

Electroplating deposits a functional layer by electrolysis or vacuum coating. PVD titanium coating gives gold, black titanium, rose gold and other colours with high hardness, wear and corrosion resistance — the first choice for luxury boutiques. Broken down below along the wet-plating and vacuum-coating routes.

6.1 Process Flow

Plating splits into wet electroplating and vacuum coating (PVD). PVD titanium is deposited by target sputtering in vacuum: film 0.3–0.5 μm, hardness HV 1500–2500, in gold, champagne, black titanium, rose gold and blue titanium. Anodising is mainly for aluminium, giving a wear- and weather-resistant oxide film.

  • Step 01 · Pre-treatment cleaning — degrease → pickle → DI rinse
  • Step 02 · Drying & loading — dust-free / dew-point control
  • Step 03 · Ion bombardment — Ar ion cleaning
  • Step 04 · Film deposition — target sputtering / arc evaporation
  • Step 05 · Cooling & unloading — vacuum-cool to 60 ℃
  • Step 06 · Inspection & film — film / ΔE / adhesion

6.2 Sub-Process Breakdown

Pre-treatment

  • 01-1 Ultrasonic degreasing — alkaline degreaser pH 9–11 · 50–60 ℃ · ultrasonic 3–5 min · two rinse stages
  • 01-2 Acid activation — weak-acid soak 1–3 min · removes the oxide film · activates the surface · DI-water rinse
  • 01-3 DI-water rinse & drying — DI-water rinse conductivity ≤ 10 μS/cm · drying 80–120 ℃ · transfer in dust-free conditions · dew point ≤ −40 ℃

Coating

  • 03-1 Ion bombardment cleaning — Ar ion bombardment · vacuum level ≤ 5×10⁻³ Pa · bias voltage 300–800 V · time 5–15 min
  • 04-1 Film deposition — targets Ti / Cr / Zr · arc current 60–120 A · deposition temperature 150–450 ℃ · film 0.3–0.5 μm
  • 06-1 Inspection & film — thickness gauge 0.3–0.5 μm · colorimeter ΔE ≤ 1.0 · cross-cut adhesion class 0 · PE film protection

6.3 Key Parameters

  • Pre-treatment conductivity — ≤ 10 μS/cm
  • Vacuum level — ≤ 5×10⁻³ Pa
  • Ion-bombardment bias — 300–800 V
  • Arc current — 60–120 A
  • Coating temperature — 150–450 ℃
  • Film — 0.3–0.5 μm
  • Hardness — HV 1500–2500
  • Adhesion — cross-cut class 0
  • Salt spray — ≥ 500 h
  • Colour difference — ΔE ≤ 1.0
  • Anodised film — 10–25 μm
  • Anodising voltage — 12–20 V

6.4 Control Points

  • Pre-treatment decides adhesion — eight out of ten PVD failures come from incomplete pre-treatment. Multi-stage ultrasonic cleaning is mandatory, with DI-rinse conductivity ≤ 10 μS/cm.
  • One furnace, one colour — one colour code must be coated in one furnace run; target wear shifts colour, so targets need scheduled replacement.
  • Film uniformity — parts must rotate in the chamber so all faces coat evenly, deviation ≤ ±15%.
  • Colour-difference control — keep a colour board per furnace and colorimeter-sample panels; deliver only at ΔE ≤ 1.0.
  • Target management — targets must be replaced at end of life, or film composition drifts and colour shifts.
  • Cooling rate — vacuum-cool below 60 ℃ before opening the furnace; quenching cracks the film.

6.5 Equipment

  • Pre-treatment equipment — ultrasonic cleaning line · DI-rinse tank · drying oven
  • Vacuum coating equipment — multi-arc ion plating furnace · magnetron sputtering furnace · vacuum pump set
  • Anodising equipment — electrolytic tank / rectifier · temperature control system · sealing line
PVD titanium colour range: gold, champagne, black titanium, rose gold, blue titanium and bronze
PVD titanium colour range: gold, champagne, black titanium, rose gold, blue titanium and bronze

PVD titanium colour range — gold TiN · light gold · black Ti · rose gold · blue Ti · bronze. Film 0.3–0.5 μm · hardness HV 1500–2500 · salt spray ≥ 500 h · one colour code per furnace run · targets Ti/Cr/Zr · arc current 60–120 A.

PVD coating cross-section (real cut edge): substrate, transition layer, functional layer and top layer
PVD coating cross-section (real cut edge): substrate, transition layer, functional layer and top layer

PVD coating cross-section (real cut edge) — stainless substrate → transition layer → functional layer 0.3–0.5 μm → top layer (optional) 0.05–0.1 μm. Total film 0.3–0.5 μm · vacuum sputter deposition · adhesion cross-cut class 0.

Ultrasonic degreasing line: the key pre-treatment step before PVD
Ultrasonic degreasing line: the key pre-treatment step before PVD
Ion bombardment cleaning: argon plasma inside the vacuum chamber
Ion bombardment cleaning: argon plasma inside the vacuum chamber
Multi-arc ion plating furnace: film deposition
Multi-arc ion plating furnace: film deposition
Anodising line: oxide film formation on aluminium
Anodising line: oxide film formation on aluminium
Coating inspection: film thickness, colour difference and adhesion
Coating inspection: film thickness, colour difference and adhesion

7. Process Selection Matrix for the Three Scenes

The same process fits the three scenes very differently. The matrix below rates each cell by usage frequency and recommendation, for a quick read of which process combination suits which scene.

7.1 Spray

  • Luxury boutique — support · aluminium recolour
  • Premium residence — common · matte plain
  • Luxury hotel — large areas · fluorocarbon
  • Typical gloss — 4 – 40 GU
  • Colour capability — full range · adjustable
  • Wear resistance — medium · coating repairable
  • Weatherability — excellent · fluorocarbon ≥ 20 years
  • Cost band — medium · priced by area
  • Repairability — excellent · spot repainting
  • Typical applications — aluminium facades / shaped columns

7.2 Polish

  • Luxury boutique — core · 8K mirror
  • Premium residence — use with care · too reflective
  • Luxury hotel — local · lift lobbies
  • Typical gloss — 48 – 96 GU
  • Colour capability — base colour only · unchanged
  • Wear resistance — low · scratches easily
  • Weatherability — good · mainly indoor
  • Cost band — medium-high · labour-intensive
  • Repairability — poor · needs full re-polish
  • Typical applications — storefronts / display cases

7.3 Brush

  • Luxury boutique — support · local texture
  • Premium residence — core · long-grain brushed
  • Luxury hotel — core · AF brushed
  • Typical gloss — 30 – 55 GU
  • Colour capability — base colour only · unchanged
  • Wear resistance — medium · grain hides scratches
  • Weatherability — good · mainly indoor
  • Cost band — medium · highly automated
  • Repairability — medium · local re-brushing
  • Typical applications — wall panels / skirtings

7.4 Plate

  • Luxury boutique — core · PVD titanium
  • Premium residence — accent · local decoration
  • Luxury hotel — support · signage & hardware
  • Typical gloss — depends on substrate
  • Colour capability — gold / black Ti / rose gold etc.
  • Wear resistance — high · HV 1500+
  • Weatherability — excellent · salt spray ≥ 500 h
  • Cost band — high · equipment and target cost
  • Repairability — poor · needs re-coating
  • Typical applications — signage / hardware / grilles

Luxury boutique

Luxury boutique: PVD titanium display cases and mirror polishing
Luxury boutique: PVD titanium display cases and mirror polishing

Led by PVD titanium and mirror polishing, brushing as a supporting texture, spraying for recolouring shaped parts.

  • Combination split — PVD plating 35% · mirror polishing 30% · brushing 22% · spray recolour 13%

Premium residence

Premium residence: long-grain brushed door casings and skirtings
Premium residence: long-grain brushed door casings and skirtings

Long-grain brushing at the core, spraying for matte plain colours, plating only as local accents.

  • Combination split — brushing 50% · matte spray 25% · plating accents 15% · local polishing 10%

Luxury hotel

Luxury hotel: fluorocarbon sprayed walls and anti-fingerprint brushed metal
Luxury hotel: fluorocarbon sprayed walls and anti-fingerprint brushed metal

Fluorocarbon spraying covers large areas, brushing for anti-fingerprint zones, plating for signage and hardware.

  • Combination split — fluorocarbon spray 40% · AF brushing 36% · plated signage 15% · local polishing 9%

8. Quality Inspection Methods

Surface treatment quality cannot be judged by eye alone. Below are the inspection items, instruments and acceptance criteria for the four processes; agree the inspection plan at the sample-sealing stage.

8.1 Spray Coating Inspection

  • Film — magnetic / eddy-current gauge · 30–120 μm
  • Adhesion — cross-cut (GB/T 9286) · class 0 / ≥ 95% squares
  • Colour difference — colorimeter, D65 · ΔE ≤ 1.0
  • Gloss — gloss meter 60° · checked against sealed samples
  • Weatherability — QUV accelerated ageing · ≥ 2000 h
  • Hardness — pencil hardness · ≥ 2H

8.2 Polishing Inspection

  • Roughness — profilometer · Ra 0.01–0.8 μm
  • Gloss — gloss meter 60° · 12–96 GU
  • Flatness — 1 m straightedge + feeler · ≤ 0.5 mm/m
  • Visual check — haze / rings / waviness · no visible defects
  • Reflection test — mirror face-on, no distortion · no funfair-mirror effect
  • Surface cleaning — no compound residue · no oil or fingerprints

8.3 Brushing Inspection

  • Grain direction — visual check · one direction per elevation
  • Grain depth — profilometer · Ra 0.2–1.2 μm
  • Gloss — gloss meter 60° · 30–55 GU
  • Grain uniformity — visual + raking light · no uneven depth
  • Anti-fingerprint coating — film 1–3 μm · fingerprint wipe test
  • Colour difference — colorimeter · ΔE ≤ 1.0

8.4 Plating / PVD Inspection

  • Film — X-ray gauge / step profiler · 0.3–0.5 μm
  • Adhesion — cross-cut · class 0; no flaking in bend test
  • Colour difference — colorimeter, D65 · ΔE ≤ 1.0
  • Hardness — micro-hardness tester · HV 1500–2500
  • Salt spray — neutral salt spray · ≥ 500 h
  • Wear resistance — rub tester · 1000 cycles at 500 g, no breakthrough

8.5 Common Inspection

  • Colour difference — colorimeter · ΔE within spec vs sealed samples
  • Appearance — visual · no scratches / specks / stains
  • Dimensions — caliper / tape · per fabrication ticket
  • Flatness — straightedge + feeler · per scene standard
  • Packing — PE film intact · corner guards · scannable QR
  • Batch consistency — same-batch sampling · ΔE / film / gloss

8.6 Environment & Safety

  • Booth cleanliness — particles ≤ 1000/m³ · positive pressure
  • Temperature & humidity — 20–28 ℃ · 45–65% RH
  • Wastewater treatment — neutralisation · heavy-metal precipitation · compliant discharge
  • Exhaust gas treatment — activated-carbon adsorption + catalytic combustion
  • Occupational protection — respirators / dust masks / goggles
  • Hazardous waste — sorted collection · compliant disposal · full records
Coating thickness measurement: magnetic, eddy-current and X-ray gauges
Coating thickness measurement: magnetic, eddy-current and X-ray gauges
Colour difference comparison: checked against sealed samples under a D65 source
Colour difference comparison: checked against sealed samples under a D65 source
Gloss measurement: 60° gloss meter
Gloss measurement: 60° gloss meter
Cross-hatch adhesion test: class 0 is the pass grade
Cross-hatch adhesion test: class 0 is the pass grade
Environment and safety: wastewater and exhaust gas treatment facilities
Environment and safety: wastewater and exhaust gas treatment facilities

Inspection principles — surface treatment quality must be judged against the sealed samples, compared under a D65 standard light source. Colorimeters, thickness gauges, profilometers and gloss meters are the four mandatory instruments; adhesion, salt spray and abrasion are type-test items, sampled every batch. All inspection data must be recorded and archived as the basis for acceptance and after-sales traceability.

9. Common Surface Treatment Defects and Prevention

These twelve problems account for over 90% of after-sales complaints in metal surface finishing. Spotting the causes and defending early in the process costs an order of magnitude less than reworking afterwards.

9.1 Coating peeling (spray)

Incomplete degreasing, an incomplete chromate film, or insufficient cure temperature or time leave adhesion below spec.

  • Prevention — multi-stage ultrasonic cleaning with DI-rinse conductivity ≤ 10 μS/cm; cure curves recorded and archived; cross-cut class 0 before delivery

9.2 Orange peel / sagging (spray)

Gun too close, film too thick, thinner flashing off too fast, or ambient temperature too high — the coating levels poorly.

  • Prevention — gun distance 150–250 mm; control film by multi-pass spraying; 20–28 ℃ and 45–65% RH

9.3 Specks / contamination (spray)

Poor booth cleanliness, jigs shedding old coating, or poorly filtered paint put particles in the film.

  • Prevention — positive-pressure dust-free booth with particles ≤ 1000/m³; clean jigs regularly; filter paint through 100–150 mesh

9.4 Haze / rings (polish)

Previous-grade marks not fully removed when changing grits, or wheel speed and pressure too high, overheating the surface locally.

  • Prevention — step through every grit with direction perpendicular each time; keep speed at 2000–3000 rpm; reflection-test mirrors

9.5 Surface yellowing (polish)

Excessive pressure overheats the surface and oxidises stainless yellow; copper not oxidation-protected straight after polishing.

  • Prevention — control pressure and temperature; apply AF coating or anti-oxidation sealing immediately after polishing

9.6 Waviness (polish)

An uneven wheel face or an undressed cloth wheel puts periodic waves in the surface.

  • Prevention — dress wheel faces regularly; replace cloth wheels at end of life; keep buffing pressure even

9.7 Mismatched grain direction (brush)

Panels on the same elevation brushed in different directions, or grain not flowing across joints — reflections clash badly at different angles.

  • Prevention — mark grain direction on the fabrication ticket; one direction per elevation; grain must flow across seams

9.8 Uneven grain depth (brush)

Belts used past their life give shallower grain; unstable feed speed gives uneven depth.

  • Prevention — log belt hours and replace on schedule; hold feed speed at 3–8 m/min; compare grain depth panel by panel

9.9 Fingerprint residue (brush)

No AF coating after brushing, or the coating is too thin, so fingerprints will not wipe off.

  • Prevention — apply 1–3 μm AF coating after brushing; cure it fully; supply neutral detergent and microfibre cloths

9.10 Film peeling (PVD)

Incomplete pre-treatment cleaning, insufficient vacuum, film too thin, or later attack by strong-alkali or chlorine cleaners.

  • Prevention — multi-stage ultrasonic cleaning with conductivity ≤ 10 μS/cm; vacuum ≤ 5×10⁻³ Pa; film ≥ 0.3 μm; supply a neutral-cleaner list

9.11 Colour drift (PVD)

Different target wear between furnace runs, temperature fluctuation, or part position in the chamber shift the colour.

  • Prevention — one colour code per furnace run; replace targets on schedule; rotate parts for uniformity; keep a colour board per furnace at ΔE ≤ 1.0

9.12 Uneven film thickness (PVD)

Parts not rotating, unequal target-to-part distances, or arc-current fluctuation give uneven film across faces.

  • Prevention — rotating jigs; control target-to-part distance; stable arc current; film deviation ≤ ±15%
Coating peeling: incomplete pre-treatment or insufficient curing
Coating peeling: incomplete pre-treatment or insufficient curing
Orange peel and sagging: film too thick or gun too close
Orange peel and sagging: film too thick or gun too close
Haze and rings: previous-grade marks not fully removed when changing grits
Haze and rings: previous-grade marks not fully removed when changing grits
Mismatched grain direction: brushing direction not unified on the same elevation
Mismatched grain direction: brushing direction not unified on the same elevation
Fingerprint residue: no anti-fingerprint coating applied
Fingerprint residue: no anti-fingerprint coating applied
PVD film peeling and colour drift
PVD film peeling and colour drift

Core principle — the final result of surface finishing is decided 70% by pre-treatment, 20% by process parameters and 10% by equipment precision. Spray adhesion, plating bond, mirror quality and brushing uniformity all trace back to thorough pre-treatment and stable parameters. Pre-treatment must be standardised, cure curves recorded and archived, and batch colour difference instrument-checked — all three are indispensable.